On this page
The machines that print the smallest features on today's chips use light of wavelength 13.5 nm, called extreme ultraviolet or EUV. You might expect them to focus it with lenses, like a camera or a projector. They cannot. There is no glass that lets 13.5 nm light through, so every optic in the machine is a mirror, and every mirror is built from dozens of layers a few nanometres thick. Why it has to be this way is a neat piece of Class 12 optics: photon energy, thin-film interference and the resolution limit λ/NA.
Why can't EUV machines use lenses?
Start with the photon energy. E = hc/λ, and with hc ≈ 1,240 eV nm:
E = 1,240/13.5 ≈ 92 eV
That is far more than visible light (about 2 to 3 eV) and enough to be absorbed strongly by the electrons in any material, including glass and air. ASML, which builds these machines, notes that its 193 nm DUV light comes from an ArF laser, while the 13.5 nm light is made by hitting tiny droplets of molten tin with laser pulses: a weak pulse flattens each droplet and a strong pulse turns it into a plasma that emits EUV. ASML gives the droplets as about 25 microns across, repeated 50,000 times a second. It is not an X-ray tube.
Because air absorbs it, the whole beam path is in vacuum. ZEISS, which makes the optics, states that EUV systems must operate in a vacuum using only mirrors because air and glass absorb the light. How a chip fab fits these machines into the whole process is described in how semiconductor chips are made.
Why does one polished surface reflect almost nothing?
At these wavelengths every material has a refractive index very close to 1. The CXRO optical constants database at Berkeley Lab gives, at 13.5 nm, a real part of about 0.924 for molybdenum and 0.999 for silicon. (Values below 1 are normal here.)
At normal incidence the reflected amplitude at a boundary is r = (n₁ − n₂)/(n₁ + n₂). For a Mo–Si boundary:
r = (0.999 − 0.924)/(0.999 + 0.924) ≈ 0.039
The reflected intensity is r² ≈ 0.0015, only 0.15%. One boundary is useless as a mirror. But a stack of boundaries can work, if all the weak reflections arrive in step.
How does a multilayer mirror add up weak reflections?
This is thin-film interference with many films. Alternate two materials with different indices, Mo and Si, and repeat the pair many times. Call the thickness of one pair the period d.
Light reflected from the top of one pair and from the top of the next pair differs in path by 2d cos θ, where θ is the angle from the normal. For every reflection to add in phase, that path difference must be a whole wavelength:
2d cos θ = λ, so d = λ/(2 cos θ)
This is the same condition as Bragg reflection from crystal planes, and the same idea as the periodic grating in a fibre Bragg grating.
Worked example:
Normal incidence. d = 13.5/2 = 6.75 nm.
At 6° from the normal. d = 13.5/(2 cos 6°) = 13.5/1.989 = 6.79 nm.
Correction for refraction. Inside the stack the light travels in material whose average index is about 0.97 (40% Mo, 60% Si by thickness), so the condition is really 2n̄d = λ, which gives about 6.97 nm. Real mirrors sit between these values. Our own thin-film calculation with the CXRO constants finds the highest reflectance at d ≈ 6.9 nm with 40% Mo.
How many pairs? If the reflections simply added, each pair contributes two boundaries of amplitude 0.039, so about 1/(2 × 0.039) ≈ 13 pairs would bring the total amplitude to 1. A proper calculation (which accounts for light being used up as it is reflected) gives a slower rise: with no absorption, 13 pairs give about 53% and 40 pairs about 98%.
Absorption sets the ceiling. Molybdenum absorbs, so deep layers barely contribute. Including absorption, the same calculation levels off at about 74% beyond 40 to 50 pairs. Real mirrors lose a little more at rough, mixed interfaces.
What do real mirrors reach? In Optical Engineering (2002), Bajt and colleagues at Lawrence Livermore reported Mo–Si multilayers with 70% reflectance at 13.5 nm using 50 bilayers. ZEISS describes its coatings as reflecting up to 70%.
How much light survives ten mirrors?
A mirror that reflects 70% loses 30% at every bounce, and losses multiply. Suppose the light meets ten mirrors between source and wafer. That count is illustrative; the actual number depends on the machine design.
After one mirror: 0.70.
After two: 0.70² = 0.49.
After five: 0.70⁵ = 0.17.
After ten: 0.70¹⁰ = 0.028, about 2.8%.
After eleven: 0.70¹¹ = 0.020, about 2.0%.
So only a few per cent of the EUV light that enters the optics reaches the wafer. Each mirror's lost energy ends up as heat. That is why EUV sources must be so bright and why a 1% gain in mirror reflectance matters: over ten mirrors, 71% instead of 70% gives 0.71¹⁰/0.70¹⁰ ≈ 1.15, about 15% more light.
Why go to all this trouble?
Because resolution scales with wavelength. The smallest feature a lithography machine can print is
CD = k₁ λ/NA
where NA is the numerical aperture of the projection optics and k₁ is a process factor, typically around 0.3. k₁ is not a constant of nature; it depends on the resist, the mask and the tricks used. The same λ/NA scaling explains why a Blu-ray disc holds more than a DVD.
With k₁ = 0.3:
DUV immersion, 193 nm, NA 1.35. CD = 0.3 × 193/1.35 ≈ 42.9 nm.
EUV, 13.5 nm, NA 0.33. CD = 0.3 × 13.5/0.33 ≈ 12.3 nm.
High-NA EUV, 13.5 nm, NA 0.55. CD = 0.3 × 13.5/0.55 ≈ 7.4 nm.
These match the manufacturer's figures well. ASML lists its NXT:2100i immersion scanner at NA 1.35 with resolution of 38 nm or better (k₁ ≈ 0.27), and says its EUV systems went from NA 0.33 to 0.55, with a smallest feature of 13 nm and then 8 nm (k₁ ≈ 0.32).
The wavelength drops by a factor of 193/13.5 ≈ 14, which more than pays for the smaller NA that mirrors allow and the light lost along the way.
To see how weak reflections from many layers build into a strong one, try the Simulation Lab. For thin-film and Bragg problems, the Fermi Problem Library has a step-by-step solver that explains the reasoning.
Quick checklist
A 13.5 nm photon carries about 92 eV and is absorbed by glass and air, so EUV optics are mirrors in vacuum.
One Mo–Si boundary reflects only about 0.15% of the intensity (amplitude 0.039).
Reflections add in phase when 2d cos θ = λ: d = 6.75 nm at normal incidence, about 6.9 nm after the refraction correction.
Absorption caps real Mo–Si mirrors near 70%, reached with roughly 40 to 50 pairs.
Ten mirrors at 70% pass 0.7¹⁰ ≈ 2.8% of the light.
CD = k₁λ/NA: about 43 nm for 193 nm immersion, 12 nm for EUV at NA 0.33, 7 nm at NA 0.55.