On this page
A household LPG alarm has to notice a few thousand parts per million of propane and butane in kitchen air. Many such alarms use a tiny piece of tin dioxide, SnO₂, kept hot by a heater. In clean air it conducts poorly; when LPG arrives, its resistance falls by more than ten times. The physics behind that drop is the same as in your Class 12 semiconductor chapter: an n-type material, a depletion layer and an energy barrier that electrons must climb, with the Boltzmann factor deciding how many get over.
Why does tin dioxide conduct poorly in clean air?
Tin dioxide is an n-type semiconductor. A small fraction of its oxygen sites are missing, and each defect gives free electrons to the conduction band. If you are unsure why that leaves the crystal neutral overall, see why an n-type semiconductor is not negatively charged.
The sensing layer is not a single crystal. It is a porous film of tiny grains touching each other. The manufacturer Figaro explains the operating principle of its MOS-type sensors in two steps:
When tin dioxide grains are heated in air, oxygen sticks to the grain surfaces by capturing free electrons, forming negative oxygen ions.
With electrons pulled to the surface, the region just inside each grain is left with few free electrons: a depletion layer. Figaro says that in clean air this stops the current from flowing freely.
At the point where two grains touch, both depletion layers meet. An electron crossing from one grain to the next has to climb an energy barrier of height eV_b. This is the same kind of barrier you meet at a metal–semiconductor contact, explained in Walter Schottky and the Schottky diode. A zinc oxide varistor has barriers like this at its grain boundaries too, but there a large voltage breaks them down, as worked in how a surge protector's varistor clamps a voltage spike. In the gas sensor, chemistry changes the barrier instead.
What happens when LPG reaches the hot sensor?
LPG is mostly propane and butane, both reducing gases. On the hot surface they react with the adsorbed oxygen ions and are oxidised. Figaro's description: the surface density of adsorbed oxygen decreases, electrons are released back into the tin dioxide, and current flows more freely.
Fewer surface oxygen ions means a thinner depletion layer and a lower barrier. More electrons can now cross each grain boundary, so the resistance of the whole film drops. When the gas clears, oxygen re-adsorbs and the resistance recovers.
The heater is essential: Figaro's explanation starts from grains heated in air at high temperature. The datasheet below specifies a heater power of 280 mW and a preheating period of 4 days before the sensor is tested.
How does the sensor's resistance change with gas concentration?
Figaro's TGS2610-D00 LP gas sensor datasheet gives the numbers you need:
R₀ is the sensor resistance in 1,800 ppm of iso-butane, which lies between 1.2 and 12.0 kΩ from one sensor to another.
The sensitivity, Rs(3,000 ppm) / Rs(1,000 ppm), lies between 0.37 and 0.60.
On its sensitivity graph, the clean-air line sits at roughly 18 times R₀ (read from the graph, so approximate).
The same datasheet shows that the sensor also responds to hydrogen, and that its reading changes with room temperature and humidity.
Over a limited range the curve is close to a power law, Rs = R₀ (C / 1,800 ppm)^(−α). This is a fit for one part, not a law of nature. If tripling the concentration halves the resistance (a ratio of 0.50, inside the datasheet range), then 3^(−α) = 0.50, so α = ln 2 / ln 3 = 0.63.
Worked example. Take an illustrative sensor with R₀ = 5.0 kΩ.
Clean air. Rs ≈ 18 × 5.0 = 90 kΩ.
1,000 ppm. Rs = 5.0 × (1,000/1,800)^(−0.63) = 5.0 × 1.45 = 7.2 kΩ.
3,000 ppm. Rs = 7.2 × 0.50 = 3.6 kΩ.
5,000 ppm. Rs = 5.0 × (5,000/1,800)^(−0.63) = 2.6 kΩ.
How the circuit reads it. The datasheet's measuring circuit puts the sensor in series with a load resistor R_L across a supply V_C and measures the voltage across R_L. That is a potential divider: V_out = V_C R_L / (Rs + R_L). With an illustrative V_C = 5.0 V and R_L = 5.0 kΩ, V_out is 0.26 V in clean air, 2.04 V at 1,000 ppm, 2.90 V at 3,000 ppm and 3.28 V at 5,000 ppm.
This is a textbook divider sum, not a build guide. Home gas alarms are certified products tested against safety standards; a hobby module is not a substitute.
How much gas is dangerous? NIOSH lists the lower explosive limit of propane as 2.1% and of butane as 1.9% in air, so 10% of the LEL is 2,100 ppm and 1,900 ppm. The datasheet gives a typical detection range of 1–25% of the LEL.
Why does a tenfold fall in resistance need only 0.12 V less barrier?
Only electrons with enough energy to climb the barrier cross it. The fraction that can is the Boltzmann factor e^(−eV_b/kT), so the conductance goes as e^(−eV_b/kT) and the resistance as e^(+eV_b/kT).
Take two states with barriers V₁ and V₂. Then R₁/R₂ = e^(e(V₁ − V₂)/kT), so
ΔV = (kT/e) ln(R₁/R₂).
The datasheet does not state the film temperature, so take an illustrative 350 °C:
Temperature in kelvin. T = 350 + 273 = 623 K.
Thermal voltage. kT/e = (8.617 × 10⁻⁵ eV/K) × 623 K = 0.0537 V.
Tenfold fall. ΔV = 0.0537 × ln 10 = 0.0537 × 2.303 = 0.124 V.
Clean air to 1,000 ppm in the example. R falls from 90 to 7.2 kΩ, a ratio of 12.4, so ΔV = 0.0537 × ln 12.4 = 0.135 V.
Units check. kT/e is energy divided by charge, which is volts.
A barrier change of only about a tenth of a volt is enough because the dependence is exponential. Figaro's page adds that in very fine grains the depletion can spread through the whole grain, and then the Fermi level shifts instead; the same Boltzmann factor still links a tenfold change to an energy change of kT ln 10.
If the Boltzmann factor and barrier crossing still feel abstract, the Concept Library covers every concept in physics, chemistry, biology, mathematics and computing.
What should you do if you smell LPG at home?
A sensor only warns you. The LPG safety tips on the government's Pradhan Mantri Ujjwala Yojana consumer guidance say: if you smell gas, close the regulator and the burner knobs, open all doors and windows, put off all flames, do not operate electric switches, and contact your distributor. The same sheet says self repair is unsafe.
Quick checklist
SnO₂ is n-type; heated in air, adsorbed oxygen takes electrons and leaves depletion layers.
Grain boundaries become barriers of height eV_b; LPG removes oxygen and lowers them.
R ∝ e^(eV_b/kT), so ΔV = (kT/e) ln(R₁/R₂).
A tenfold fall at 623 K is a barrier change of 0.124 V.
Datasheet fit for one part: Rs(3,000)/Rs(1,000) between 0.37 and 0.60, R₀ defined at 1,800 ppm iso-butane.
The sensor needs its heater and is affected by other gases, temperature and humidity.
Smell gas: follow your LPG supplier's safety steps, not a gadget.